Home/Insights/Technical
Technical

Adhesion tests: what the number actually means

Updated 24 Oct 2026

A pull-off value can look healthy and tell you nothing. Where the film breaks matters more than the MPa figure on the report.

Adhesion test results are often treated as a score: 3 MPa is worse than 6 MPa, so the second job must be better. In practice a single number without the failure mode beside it is close to meaningless. The same coating can read 4 MPa because the adhesive failed, 4 MPa because the primer let go of the steel, and 4 MPa because the topcoat split internally — three completely different diagnoses with the same headline figure.

Three methods, three different questions

  • Cross-cut (ISO 2409 / ASTM D3359). A lattice is cut through the film and tape is applied. Fast, cheap, works on thin films and on site. It answers a qualitative question — does the coating stay on when it is deliberately damaged — and it is not a strength measurement.
  • Pull-off (ISO 4624 / ASTM D4541). A dolly is glued to the coating and pulled normal to the surface. This gives a number in MPa, and it is the only method that also records where the failure occurred. For thick protective systems it is the standard field test.
  • Flexibility and impact tests. These are sometimes filed under adhesion, but they measure something else: whether the film can deform with the substrate. A coating can be flexible and poorly bonded, or rigid and well bonded.

Read the failure mode first

Every pull-off result should be reported as a pair: the stress and the location of the break. The usual notation distinguishes adhesive failure at the substrate, cohesive failure inside a coat, adhesive failure between two coats, and failure within the adhesive itself. A result of 6 MPa with 90% cohesive failure inside the primer says the bond to steel is stronger than the primer's own cohesion, which is usually good news. A result of 6 MPa with 80% failure at the primer–steel interface says the opposite: the interface is the weak link, and the number is only that high because the surrounding area held.

Why the number misleads

The most common trap is the adhesive. If the glue releases before the coating does, the reported strength is the glue's, not the coating's, and the test should be discarded rather than recorded as a pass. The second trap is location: a dolly on flat, well-prepared plate tells you about flat, well-prepared plate. The welds, edges and cut-outs that decide service life are exactly where a dolly cannot easily be glued. The third is cure: testing a film that is still reacting produces a low number that says nothing about the system, only about the schedule. The fourth is thickness — very thick or very rigid films often fail cohesively below the true interfacial strength, because the load concentrates at the dolly edge.

What a specification should require

Write the acceptance criterion as a pair: a minimum stress and an acceptable failure mode — for example a minimum value with cohesive failure preferred, and interfacial failure at the substrate not accepted regardless of the number. Require the test after full cure, at a stated temperature, with the adhesive and its curing time recorded, and with the location of each test marked on a drawing. Ten readings scattered over a tank are more useful as a map than as an average; one low value at a weld tells you where to look.

Field practice that makes results comparable

Clean and abrade the coating surface before gluing, so the adhesive bonds to paint rather than to dust. Let the adhesive cure for its full time — most field errors come from pulling too early. Align the dolly and pull steadily rather than jerking. Record the steel temperature, because a system tested at 5 °C and one tested at 30 °C are not directly comparable. And test the same system the same way across a project, so the numbers form a trend; a trend exposes drifting surface preparation long before a single failing value does.

Where it fits in the system

Adhesion testing is a diagnostic tool, not a final exam. On a zinc-rich primer such as Interzinc 52HS the cohesive strength of the zinc film may be the limiting factor; on a high-build epoxy such as Intergard 475HS the interface to the primer is usually the place to watch. Neither is a reason to demand a higher number — it is a reason to report the mode. When a result is low, the useful next step is to look at what the break exposed: contamination, a glossy surface, a missed recoat window, or simply insufficient cure. Specific acceptance values belong to the project specification and the manufacturer's guidance in the latest TDS; publicly available manufacturer materials are the reference, and they rarely support a single pass/fail number without a failure mode.

Sources

  • ISO 4624, public scope (pull-off test for adhesion)
  • ISO 2409, public scope (cross-cut test)
  • ASTM D4541, public scope (pull-off strength of coatings using portable adhesion testers)
  • ASTM D3359, public scope (measuring adhesion by tape test)
  • ISO 12944-7, public scope (execution and supervision of paint work)
  • Publicly available manufacturer materials — zinc-rich primers, high-build epoxies and their technical data sheets

Articles are compiled by RichTech from publicly available manufacturer materials and field practice, for selection reference only; the latest official technical data sheets (TDS) prevail.

Not sure which product fits? Tell us the substrate and service conditions

Share your substrate, corrosivity category and target service life — we will come back with a coating system and quantity estimate.

Contact us